Short answer

Sink marks and voids come from the same root cause: a thick section that cures and shrinks unevenly. Silicone cures from the wall inward, so the surface freezes while the core is still shrinking — the skin pulls inward (a sink) or the core tears apart (a void). The fix is design, not more pressure: core out the thick section and keep wall thickness uniform.

Sink and void in a thick sectionUneven cure in a thick wall causes a surface sink or an internal void.thick sectionthick bossthin wallthin wallsinkvoidSkin freezes first, core still shrinks → sink or void.Fix: keep walls uniform, core out bosses to ~60–70%.
A thick section freezes on the surface while the core shrinks, pulling a sink or tearing a void — core it out instead.

Sink vs void — same cause, opposite sign

A sink mark is a shallow depression on the surface where the frozen skin was pulled down into a still-shrinking core. A void is an internal cavity where the shrinking core pulled itself apart. Both happen in the same place: a thick region surrounded by thinner walls.

Why silicone is prone to it

Silicone cures from the heated mold wall inward, and it shrinks 2–3% as it crosslinks. In a thick section, the outer skin cures first and can no longer follow the core as it shrinks — so the geometry has to give somewhere. Pressure can hold the surface flat briefly, but it cannot remove the underlying shrinkage.

Design rules that remove it

  • Keep adjacent walls within roughly 1.5:1 — a 5 mm boss on a 1 mm wall is the classic trap.
  • Core out bosses and ribs to about 60–70% of the nominal wall.
  • Blend thickness changes with radii, never an abrupt step.
  • Vent the end of fill so trapped air does not become an extra void.