Compression set is the single most important durability metric for a silicone seal, gasket or O-ring. It measures how much the part fails to recover after being squeezed — and when it fails to recover, the seal leaks. ASTM D395 is the standard test, and this guide explains how it works and what to specify.

Compression setA seal that stays compressed after load is removed.originalcompressedafter releaseh₀loadh₁ < h₀Compression set = how much thickness is not recovered.A seal that stays squashed leaks — low set = long life.
Compression set measures how much thickness a part fails to recover after load — the key test that predicts whether a seal keeps sealing.
Compression setA seal that stays compressed after load is removed.originalcompressedafter releaseh₀loadh₁ < h₀Compression set = how much thickness is not recovered.A seal that stays squashed leaks — low set = long life.
Compression set measures how much thickness a part fails to recover after load — the key test that predicts whether a seal keeps sealing.

What compression set measures

A part is compressed to a set thickness, held for a defined time at a defined temperature, then released. The compression set is the percentage of the original compression that does not recover:

Compression set % = (original thickness − recovered thickness) ÷ (original thickness − compressed thickness) × 100

A value of 0% means full recovery; 100% means the part stayed fully squashed. Lower is better for anything that must keep sealing.

ASTM D395 Method A vs Method B

  • Method A — constant force: a fixed load is applied. Used less often for seals.
  • Method B — constant deflection: the part is compressed to a fixed strain (usually 25%) for the duration. This is the standard for O-rings and gaskets.

Test conditions that matter

The result is meaningless without the conditions, so always state them. Typical conditions are 22 h, 70 h or 168 h at 23 °C, 70 °C, 100 °C, 125 °C, 150 °C, 175 °C or 200 °C. A number run at 23 °C cannot be compared with one run at 150 °C — higher temperature always makes recovery worse.

Typical silicone compression set values

CompoundCompression set (Method B, 22 h @ 100 °C)
Platinum-cured LSR5–15%
Peroxide-cured HCR15–25%
FVMQ (fluorosilicone)10–20%

Why platinum cure wins on compression set

Platinum-catalyzed addition cure cross-links the network more completely and leaves essentially no reaction by-products. The result is a denser, cleaner network that springs back after load. Peroxide cure leaves acidic by-products and a less complete network, so its recovery — and therefore its compression set — is worse. This is exactly why medical and precision seals are specified platinum-cured.

How to spec compression set on your drawing

Don't just write "low compression set". Write something like:

Compression set ≤ 15%, ASTM D395 Method B, 25% deflection, 22 h @ 100 °C

That single line tells the factory exactly which test to run and what bar to clear — and it is the line we verify on first-article and batch testing.

FAQ

What is a good compression set for silicone? For a sealing application, ≤15% is good (platinum-cured), and ≤10% is excellent. Peroxide-cured HCR typically runs 15–25%.

What is the difference between ASTM D395 Method A and B? Method A applies a constant force; Method B applies a constant deflection (typically 25%). Method B is the more common and more repeatable for seals.

Does hardness affect compression set? Generally yes — higher-durometer compounds usually show lower compression set because the denser network recovers better. But cure system matters more than hardness.

Why does peroxide-cured silicone have higher compression set? Peroxide cure leaves residual by-products and a less complete network; platinum cure cross-links more fully and cleanly, so it recovers better after load.